Welding Process Of Copper Tube And Copper Tube

May 08, 2021

Before heating, apply flux to the part to be welded.

After heating, insert the copper tube and sleeve, and move the flame nozzle back and forth continuously between the two points. Do not touch the flame directly with the flux. The temperature of steel pipe is slightly higher than that of copper pipe.

When the copper tube is heated and the flux melts into liquid, the preheated electrode is immediately placed on the solder joint. As soon as the electrode begins to melt, the flame nozzle moves back and forth between the two tubes until the solder flows into the gap between the two tubes.

Remove the flame and allow the solder to contact the solder joint for a few seconds before removing. If it is suspected or found that there is still a gap between the two tubes, it can be heated again to make the flame nozzle move continuously at two points. A small amount of solder can be added if necessary.

Ensure that the pipeline does not leak, the welding pipeline is horizontal and vertical, and the welding fluid is evenly distributed in the weld. Ensure that the function of each component is intact, and pay attention to the direction of each valve.

Copper pipe blanking A. tools: pipe cutter, tape, wire number pen, file B. steps: ① measure the corresponding length with tape according to the size and pipe diameter required in the drawing, and note down the position with wire number; ② after the thicker copper pipe is fixed, remove it with the cutter to ensure that the cutting edge is flush and not deformed; ③ file the rough edge of the cutting edge with a file, and wipe it clean with a rag.

Welding A. tools: welding gun, acetylene cylinder, oxygen cylinder, nitrogen cylinder B. steps: ① check whether the quantity in oxygen cylinder and acetylene cylinder is enough; ② carry out welding according to the drawing requirements; ③ when welding solenoid valve, the coil of solenoid valve shall be removed to prevent damage and pay attention to its flow direction; ④ weld other parts, such as liquid mirror, expansion valve Attention should be paid to the heat damage of one-way valve during welding. If necessary, the detachable parts can be removed and the welded valve body can be wrapped with wet cotton cloth. During welding, low speed nitrogen should be put into the welded pipe to prevent oxidation. After welding, cool down and clean the oxide and welding slag in the pipe with dry nitrogen.

Objective to specify the welding materials and welding methods, so as to ensure the quality of welding and ensure that there is no leakage point in the system.

Braze welding is adopted for the welding of copper pipe, the brand of welding rod is bag10cuzn, and the flux is borax. Brass welding rod is adopted for the welding of dissimilar materials, and the specification of welding rod shall be determined according to the size of the weldment.

All plug-in welding in this process shall be carried out according to the following figure. The clearance after welding and before welding is 0.1-0.25mm h ≈ D note: H is the insertion depth and D is the pipe diameter

During welding, when the copper pipe is annealed after welding, the annealing temperature shall not be lower than 300 ℃.

In the process of pressure test, repair welding should be carried out when leakage is found in the welding. During repair welding, the nitrogen of the system should be discharged, and the pressure test should be carried out again after welding.

The oxide layer on the surface shall be cleaned with gauze before repair welding. After repair welding, the oxide scale shall be removed. After quenching in water, the copper pipe shall be dried without water drops.

After all welding, the system should be blown clean with nitrogen.

Joints that are not allowed to be welded due to technical requirements shall be connected by bolts or flanges.

For the parts which are easy to deform and damage under high temperature, corresponding protection measures should be taken. For example, the corner valve, evaporator and condenser should be welded after the interface is wrapped with wet gauze. For the solenoid valve, expansion valve and liquid mirror, those that can be disassembled must be disassembled and welded. For those that cannot be disassembled, the above measures should also be taken.


Send Inquiry